Skip to main content
. 2013 Jan 28;6:15. doi: 10.1186/1754-6834-6-15

Table 4.

Cellulose DP before and after DA and hydrothermal pretreatments for different substrates

Substrate Pretreatment conditions DP before pretreatment DP after pretreatment Reference
Corn stover
DA pretreatment: 3% H2SO4, 180°C, 90 s
7300a
2700a
[32]
Poplar
DA pretreatment: 2% H2SO4, 190°C, 70 s
3500a
600a
[32]
Loblolly pine
DA pretreatment: 1% H2SO4, 180°C, 30 min
3642b
1326b
[95]
Switchgrass
DA pretreatment: 5% H2SO4, 180°C, 5 min
1891b
1342b
[82]
Corn stover
Hydrothermal pretreatment: 190°C, 15 min
7300a
5700a
[32]
Poplar Hydrothermal pretreatment: 200°C, 10 min 3500a 1750a [32]

a: DP was measured by viscometric method [96].

b: DP was measured by gel-permeation chromatography (GPC) technique [97].