Comparison of electromechanical coupling factor kij and piezoelectric coefficient dij(pC/N) for “2R” domain engineered PIN-PMN-PT:Mn, PIN-PMN-PMN, and PMN-PT crystals.

  d15 (pC/N) d24 (pC/N) d31 (pC/N) d32 (pC/N) d33 (pC/N) k15 k24 k31 k32 k33 kt
2R (A) a 2030 125 455 −1200 810 0.90 0.32 0.64 0.86 0.86 0.45
2R (B) a 2986 160 608 −1508 1053 0.92 0.34 0.71 0.90 0.90 0.46
PIN-PMN-28%PT b 2203 114 460 −1156 782 0.90 0.30 0.67 0.86 0.87 0.49
PIN-PMN-32%PT b 3354 162 744 −1781 1363 0.95 0.36 0.75 0.90 0.92 0.50
PMN-28%PT c 2816 234 723 −1761 1766 0.90 0.30 0.65 0.89 0.91 0.50
PMN-30%PT c 3262 289 813 −2116 1916 0.95 0.36 0.71 0.94 0.92 0.52
a

This work.

b

Reference 19.

c

Reference 20.