Table 2.

Nitric oxide release from coatings doped at 18 mg/mL PROLI/NO as a function of polyurethane topcoat.

NO release properties Type of polyurethane topcoat

HP 93A HPU HPU/TPU TPU TP-470
[NO]max (pmol cm−2 s−1) 3128 ± 716 2895 ± 435 2617 ± 395 1526 ± 234 1436 ± 261
tmax (min) 8.4 ± 0.8 8.4 ± 0.6 9.1 ± 0.5 18.0 ±1.2 16.8 ± 2.5
[NO]6 h (pmol cm−2 s−1) 5.45 ± 2.38 6.72 ± 2.19 23.47 ± 3.91 28.49 ± 3.69 26.53 ± 4.45
[NO]12 h (pmol cm−2 s−1) 0 1.85 ± 0.23 2.54 ± 0.36 5.67 ± 0.71 6.89 ± 0.80
[NO]24 h (pmol cm−2 s−1) 0 0 0.94 ± 0.32 1.67 ± 0.30 1.96 ± 0.26
Total NO (μmol cm−2) 3.9 ± 0.4 3.8 ± 0.5 4.1 ± 0.5 4.2 ± 0.5 4.1 ± 0.4