Skip to main content
. Author manuscript; available in PMC: 2014 Oct 1.
Published in final edited form as: Biomaterials. 2013 Jul 13;34(31):7766–7775. doi: 10.1016/j.biomaterials.2013.06.039

Table 1.

Numerical summary of swelling and antibody recovery from variable silk density lyogels

Sample Silk density
(mg (cm3)−1)
Swelling ratio Antibody
recovery (%)
3.1% silk 51.6 (±2.6) 16.0 (±0.6) 81.3 (±7.7)
4.3% silk 56.4 (±2.7) 13.8 (±1.6) 74.2 (±2.3)
5.5% silk 63.3 (±1.8) 9.1 (±0.9) 52.2 (±3.5)
6.7% silk 80.4 (±5.1) 6.7 (±0.3) 36.0 (±2.0)
Not pressed 44.9 (±3.7) 14.5 (±1.0) 69.8 (±7.2)
1500 psi 1045.3 (±36.8) 0.6 (±0.01) 15.6 (±1.6)
2500 psi 1320.5 (±40.5) 0.5 (±0.08) 3.0 (±0.6)