Skip to main content
. Author manuscript; available in PMC: 2014 Apr 1.
Published in final edited form as: Biomaterials. 2013 Jan 23;34(11):2577–2587. doi: 10.1016/j.biomaterials.2012.12.028

Table 1.

Summarizes the results of the stepped, static mechanical testing.

Collagen type Starting concentration (mg/ml) Samples tested Flow rate Polyethylene glycol concentration (wt/wt%) Average # of monomers per 300 nm Single monomer cross-sectional area (μm2) Total collagen cross-sectional area (μm2) Modulus at 2% strain (MPa)
Telo 1.8 pH 2.0 6 100% 30% pH 7.3 6.74E+06 1.77E-06 11.92 12.3 ± 1.13
Atelo 6 10.2 ± 0.82
6 75% 5.06E+06 8.94 14.6 ± 0.61
6 50% 3.37E+06 5.96 17.3 ± 1.16
7 100% 35% pH 7.3 6.74E+06 11.92 16.5 ± 2.12
6 75% 5.06E+06 8.94 17.3 ± 2.37
6 50% 3.37E+06 5.96 22.5 ± 3.25