Skip to main content
. 2013 Sep 24;12:95. doi: 10.1186/1475-925X-12-95

Table 2.

DSC results for aged and non aged HDPE and HA/HDPE composites

Non aged specimens
Aged specimens
  Xc% 0 kGy Tm (°C) Xc% 35 kGy Tm (°C) Xc% 70 kGy Tm (°C) Xc% 0 kGy Tm (°C) Xc% 35 kGy Tm (°C) Xc% 70 kGy Tm (°C)
HDPE + 0% HA
54 ± 1.8
134
60 ± 2.1
134.8
63 ± 1.8
135
59 ± 2.2
131.9
62 ± 2.2
132.1
63 ± 2.3
132.6
HDPE + 10% HA
51 ± 1.3
133
58 ± 2.1
133.2
59 ± 2
133.9
57 ± 1.8
131.6
59 ± 2.25
132.4
61 ± 2.25
132.8
HDPE + 20% HA
50 ± 1.31
132.3
54 ± 1.66
132.7
56 ± 1.6
133.2
52 ± 1.65
130.5
54 ± 1.58
131
58 ± 1.95
132