Skip to main content
. 2014 Jan 9;4:3620. doi: 10.1038/srep03620

Table 1. Electrochemical parameters of the samples derived from polarization tests in 0.9 wt.% NaCl.

Sample Immersed time Ecorr (mV) Icorr (mA cm−2) EPP (mV) ACR(mm y−1)
MDZ-C 10 min −1600 0.1011 −1453 2.3344
  2 h −1546 0.1308 −1310 3.0202
  4 h −1507 1.0421 −1213 24.062
MDZ-545 10 min −1605 0.0951 −1303 2.1951
  2 h −1571 0.0862 −1303 1.9904
  4 h −1516 0.0461 −1303 1.0645