Published in final edited form as: Pharm Res. 2014 Feb;31(2):436–448. doi: 10.1007/s11095-013-1173-6

Table 5.

Summary of initial rate constants for polymer degradation in blank implants and in implants with encapsulated lysozyme, with or without MgCO3, measured by GPC.

Polymer Name Lysozyme (%) MgCO3 (%) Initial rate constant (day -1)
AB10 0 0 0.075±0.003
AB15 0 0 0.104±0.002
ABA10 0 0 0.116±0.002
PLGA 0 0 0.120±0.002
AB10-PLGA a 0 0 0.110±0.002
AB15-PLGA a 0 0 0.117±0.004
AB10 15 0 0.047±0.002
AB10 15 3 0.050±0.003
AB15 15 0 0.023±0.001
AB15 15 3 0.039±0.002
ABA10 15 0 0.094±0.002
ABA10 15 3 0.053±0.002
PLGA 15 0 0.034±0.003
PLGA 15 3 0.015±0.001
AB10-PLGA a 15 0 0.050±0.006
AB10-PLGA a 15 3 0.029±0.003
AB15-PLGA a 15 0 0.056±0.003
AB15-PLGA a 15 3 0.028±0.001
a

Block copolymers were blended with PLGA 50/50 at a 1:1 w/w ratio.