Sample Mean of Thickness (μm) mean relaxation time, τ (min) Effective diffusion coefficient, Deff (mm2/s)
2PU10GE 2PU10GE-2.5′ 18.0 5.08±0.67 5.84±0.82 × 10−4
2PU10GE-5′ 20.5 7.92±2.27 4.51±1.52 × 10−4
2PU10GE-10′ 25.6 43.99±2.22 9.5±0.47 × 10−5
6PU10GE 6PU10GE-2.5′ 16.0 8.01±0.54 3.27±0.23 × 10−4
6PU10GE-5′ 17.4 21.10±3.85 1.38±0.28 × 10−4