Table 1.

Conditions for plasma-spray deposition of hydroxyapatite on titanium

Condition Parameter
Primary spray gas, Ar 40 SLPM
Secondary spray gas, H2 10 SLPM
Carrier gas, Ar 2 SLPM
Powder-flow rate 25 g/min
Plasma-jet type F4-MB
Injector size, diameter 1.8 mm
Powder-feeding distance 8 mm
Spray current 650 A
Spray voltage 58 V
Spray distance 100 mm

Abbreviation: SLPM, standard liters per minute.