Skip to main content
. 2014 Jun 17;15(6):10950–10973. doi: 10.3390/ijms150610950

Table 2.

DMA data for neat PHB and the nanocomposites with different ZnO loadings.

ZnO (wt %) Tg (°C) E'−100 °C (GPa) E'25 °C (GPa) E'100 °C (GPa) 102 tan δmax (a.u.) FWHM (°C) tan δarea (a.u.)
0 17.9 1.81 0.78 0.24 8.11 13.9 0.79
1.0 22.1 2.27 0.93 0.30 7.23 19.2 1.06
2.0 28.4 2.39 1.11 0.37 7.98 22.9 1.13
5.0 27.7 2.59 1.11 0.36 6.35 26.8 1.18
10.0 32.6 2.78 1.18 0.39 7.19 24.5 1.11

E': storage modulus; Tg: glass transition temperature; tan δmax: tan δ maximum value; FWHM: full-width at half maximum of tan δ peak; tan δarea: area under tan δ peak.