Skip to main content
. 2014 Jul 17;2014:542678. doi: 10.1155/2014/542678

Table 2.

Flexural strength mean and standard deviation (MPa) for the interaction between %wt of glass fibers and type of resinous material. Statistical comparisons by ANOVA following Tukey-HSD test and paired comparisons by Student t-test (α = 0.05).

Quantity of glass fibers (%wt) Type of resinous materials
Filled resin Unfilled resin
0 442.78 ± 140.65Ca 187.76 ± 120.37Bb
10 772.81 ± 446.33ABCa 795.48 ± 688.19Ba
15 854.78 ± 297.35ABb 1999.91 ± 1258.65Aa
20 863.46 ± 418.05Ab 1911.55 ± 596.88Aa
30 459.55 ± 140.59BCb 2090.61 ± 656.79Aa

Different capital letters (vertical analysis) and lower case letters (horizontal analysis) mean statistical significant differences with P < 0.05.