Table 5. Mechanical Properties of Films with Average Deviations after Post-Pour Stretch Using Set Ratios of IPA, MeOH, and Water.

material + stretch solutions with stretch ratio avg energy to break (MJ/m3) avg ultimate stress (MPa) avg ultimate strain (mm/mm)
MaSp1 + 50/50 IPA/water 2.5× 30.44 ± 3.55 136.66 ± 2.06 0.253 ± 0.02
MaSp1 + 80/20 MeOH/water 2.5× 40.6 ± 3.34 149.42 ± 7.27 0.335 ± 0.02
80/20 MaSp1/MaSp2 + 80/20 MeOH/water 2.5× 40.58 ± 10.9 168.35 ± 20.76 0.307 ± 0.1
80/20 MaSp1/MaSp2 + 80/20 MeOH/water 2.7× 47.06 ± 3.08 206.81 ± 3 0.289 ± 0.02
80/20 MaSp1/MaSp2 + 50/50 IPA/water 3× 52.36 ± 8.02 183.92 ± 14.85 0.354 ± 0.07
80/20 MaSp1/MaSp2 + 50/50 IPA/water 3.2× 34.58 ± 10.7 177.56 ± 3.57 0.239 ± 0.07