Skip to main content
. 2014 Sep 5;4:6294. doi: 10.1038/srep06294

Table 1. Magnetic and powder properties for each type of MagCE and for the source materials (Please also see Table S3 (detailed information for this Table), Supplementary file).

  Size Pore distribution Magnetic property
  Ave (μm) Fine pore volume (μm3/g) Specific surface area (μm2/g) Porosity (%) Hc (kA/m) σs (A·m2/kg)
Acicular iron nanoparticle - - - - 116.2 119
MagCEBAG 1.68 0.04 0.62 - 115.4 62.1
MagCE (value of rotameter (mm)) 35 10.28 0.71 1.97 62.7 113.5 60.8
  40 8.3 0.55 1.85 63.8 114.4 59.7
  45 6.51 0.44 1.78 69.1 114.4 60.3
  50 5.19 0.36 1.64 71.2 114.8 60.3
  55 4.38 0.31 1.54 71.9 114.8 60.0
Cracked powder 23.88 0.25 0.93 - 106.1 75.5
Spherical iron nanoparticle - - - - 39.8 150.3
Spherical iron nanoparticle- based MagCE 5.71 0.0011 1.72 65.1 39.3 59.6
Spherical iron oxide nanoparticle - - - - 10.3 62.8
Spherical iron nanoparticle- based MagCE 5.6 0.0022 1.65 65.3 12.5 22.7