Skip to main content
. 2014 Oct 27;2014:385135. doi: 10.1155/2014/385135

Table 1.

Characterization of microparticles with respect to mean diameter, zeta potential, mean loading, and encapsulation efficiency.

Formulation Mean diameter (nm) Zeta potential (mV) Mean loading (µg/mg) Encapsulation efficiency (%)
PLGA : A1(50 : 50) 1034 ± 22.4 −18.1 ± 1.67 1.98 ± 0.12 19.88 ± 1.2
PLGA : A1(75 : 25) 997 ± 12.5 −23.2 ± 1.5 1.49 ± 0.15 14.96 ± 1.55
PLGA : A1(85 : 15) 1882 ± 23.7 −17.5 ± 2.4 1.32 ± 0.07 13.29 ± 0.72
PLGA : A2(50 : 50) 821.2 ± 11.5 −15 ± 2.83 1.42 ± 0.09 14.28 ± 0.95
PLGA : A2(75 : 25) 1121 ± 20.1 −23.1 ± 1.09 1.14 ± 0.14 11.44 ± 1.48
PLGA : A2(85 : 15) 797.1 ± 9.88 −36.3 ± 2.47 0.98 ± 0.18 9.88 ± 1.8
PLGA alone (100 : 0) 612.9 ± 6.39 −38.1 ± 1.96 0.33 ± 0.04 3.325 ± 0.43

All the values are represented mean values of three independent experiments.