Table 1.

Electrospinning processing conditions for the PCL microfibrous scaffold and SF/PCL nano/microfibrous composite scaffolds

SF concentration (wt%) Voltage (kV) Flow rate (mL/h) TCD (cm) Needle gauge (G)
PCL 100 17 1 10 21
SF/PCL 2/98 3 7 0.8 8 24
SF/PCL 4/96 3 8 1.6 8 24
SF/PCL 6/94 3 8.5 2.4 8 24
SF/PCL 8/92 3 9 3.3 8 24

Abbreviations: PCL, poly(ε-caprolactone); SF, silk fibroin; TCD, needle tip-to-collector distance.