Table.

Means and Standard Deviations of Telopeptide of Type I Collagen (ICTP) Concentration (µg/L) in Artificial Saliva after 4 wk of Immersion and Microtensile Bond Strength (in megaPascals, MPa) to Dentin and Mode of Failure of Experimental Groups

Mode of Failure (%)
ICTP
(μg/L)
(n = 15)
μTBS
MPa
(n = 50)
A C M
Demineralized dentin 220.13 (15.32) A XX X X X
Resin 14.40 (2.12) B 32.44 (6.31) a 0 0 100
Resin with NPs 5.6 (1.02) C 28.45 (7.22) a 10 0 90
Resin with Zinc-NPs 0.1 (0.02) D 27.06 (6.77) a 5 0 95

Abbreviations: μTBS, microtensile bond strength to dentin; NPs, nanoparticles; Zinc-NPs, zinc-loaded nanoparticles; A, adhesive; C, cohesive; M, mixed. For each vertical column, values with identical letters indicate no statistically significant difference by Student-Newman-Keuls test (p > .05).