TABLE II.
Ecorr, Icorr and Epitt Readings Determined from Potentiodynamic Polarization Curves for Plasma Coatings Deposited onto 316L Stainless Steel Stents in PBS Electrolyte with Ag/AgCl Reference Electrode
Treatment | Ecorr (mV) | Icorr (μA/cm2) | Epitt (mV) |
---|---|---|---|
316L SS | –198.72 ± 22.53 | 4.09 ± 2.39 | +461.4 ± 43.1 |
DC-TMS | +76.95 ± 6.93* | 0.63 ± 0.10 | +693.3 ± 27.7* |
DC-TMS + NH3/O2 | +9.88 ± 34.37* | 2.54 ± 1.99 | +710.6 ± 9.4* |
RF-TMS | –64.58 ± 51.08* | 0.16 ± 0.05 | +612.0 ± 17.4* |
RF-TMS + NH3/O2 | –14.87 ± 50.60* | 0.12 ± 0.08 | +562.0 ± 67.6* |
The data are presented as means 6 standard deviations for n = 3.
(denotes p< 0.05, as compared to 316L SS).