Table 2.
Sample | Ecorr(mV) | Icorr(A) ×10−6 | Corrosion rate (mpy) ×10−3 | Rct (Ω) × 104 | Cdl (µF) | Protective efficiency % |
---|---|---|---|---|---|---|
316 L SS blank | −412 | 7.2 | 2.13 | 0.36 | 2.5 | – |
1.5 μm TFMG/SS | −300 | 4.8 | 1.4 | 2.25 | 1.2 | 40.85 |
3 μm TFMG/SS | −243 | 1.0 | 0.31 | 2.66 | 1.09 | 85.428 |
Abbreviations: SS, bare stainless steel; TFMG/SS, thin film metallic glass-coated stainless steel; Icorr, corrosion current density; Ecorr, corrosion potential.