Table 2.
Thin film spin-coating conditions, their root mean square (RMS) surface roughness, and FET mobilities.
| Entry | PAH | Solv. | Conc. [10−4 m] | Spin speed [rpm] | RMS roughness [nm] | Mobility [cm2 V−1 s−1] |
|---|---|---|---|---|---|---|
| 1 | 1 a | toluene | 4.5 | 2500 | 19.7 | n.a. |
| 2 | 1 a | toluene | 4.5 | 4000 | 18.4 | n.a. |
| 3 | 1 b | toluene | 4.5 | 4000 | 1.9 | 8.3×10−9 |
| 4 | 1 a | toluene | 4.5 | 5000 | 21.4 | n.a. |
| 5 | 1 a | toluene | 2.0 | 4000 | 14.5 | n.a. |
| 6 | 1 b | toluene | 2.0 | 4000 | 1.2 | 3.4×10−8 |
| 7 | 1 a | toluene | 0.5 | 4000 | 13.2 | n.a. |
| 8 | 1 a | DCB | 2.0 | 4000 | 22.7 | n.a. |
| 9 | 1 b | DCB | 2.0 | 4000 | 2.3 | 7.9×10−9 |
n.a.: not applicable