Table 3. Photovoltaic parameters of devices I, J and K measured at 50 mW cm-2, before and after aging under standard AM 1.5G illuminations at 100 mW cm-2 and 60 °C.

Device Alkyl chain Electrolyte Aging [h] JSC [mA cm–2] VOC [mV] Fill Factor PCE [%] Ecb shift Δ(Ecb Shift–VOC)
I C2 ES2 0 7.82 682 0.73 7.87 0
1000 7.91 646 0.72 7.50 36
J C3 ES3 0 7.22 688 0.74 7.49 10
1000 7.48 663 0.73 7.34 35
K C4 ES4 0 7.73 665 0.72 7.50 15
1000 7.10 643 0.70 6.45 37