Skip to main content
. 2016 Mar 7;6:22810. doi: 10.1038/srep22810

Table 2. Tensile properties of NR, SR, and natural rubber/slide-ring composites.

Test NR SR NR/SR (100/30) NR/SR (100/40) NR/SR (100/50) NR/ENR/SR (90/10/40) NR/ENR/SR (80/20/40) NR/ENR/SR (70/30/40)
Tensile Modulus at 100% strain/MPa 0.71 ± 0.04 0.01 ± 0.002 0.43 ± 0.03 0.37 ± 0.04 0.34 ± 0.04 0.39 ± 0.03 0.41 ± 0.03 0.38 ± 0.03
Tensile Modulus at 300 strain/MPa 1.83 ± 0.12 0.04 ± 0.005 1.03 ± 0.09 0.84 ± 0.06 0.84 ± 0.07 0.96 ± 0.05 1.00 ± 0.05 0.95 ± 0.07
Tensile strength /MPa 21.6 ± 0.62 0.045 ± 0.007 15.4 ± 0.41 12.5 ± 0.39 12.1 ± 0.36 13.2 ± 0.37 13.3 ± 0.33 12.9 ± 0.35
Elongation at break/% 711 ± 5.38 352 ± 3.88 776 ± 5.34 784 ± 5.61 794 ± 5.53 782 ± 5.23 788 ± 5.46 773 ± 5.44
Hardness 42 ± 0.56 15 ± 0.34 30 ± 0.67 28 ± 0.55 25 ± 0.37 29 ± 0.48 30 ± 0.39 31 ± 0.40