Table 8.

Effects of multiple layers of two self-etch adhesives on microtensile bond strength.

Layers
Groups 1 2 3 4 5 1 + SBMP
Xeno IIIf
(evaporation)
7.2 ± 6.3a 22.6 ± 9.2a,b 30.0 ± 9.9b 43.5 ± 7.7c 41.4 ± 8.0c 27.8 ± 5.9b
Xeno IIIf
(evaporation
+ 1c)
7.2 ± 6.3a 47.3 ± 19.2b 65.4 ± 20.4d 81.8 ± 20.8d 68.9 ± 22.6d 64.7 ± 21.2d
iBondi
(evaporation)
12.2 ± 7.5A 18.5 ± 6.2A 30.6 ± 7.0B 34.2 ± 6.0B,C 51.6 ± 14.8B,C 62.3 ± 23.0C
iBondi
(evaporation
+ 1c)
12.2 ± 7.1A 39.6 ± 15.2B 42.7 ± 12.3B,C 36.6 ± 7.7B 35.8 ± 13.4B 58.0 ± 23.5C

Values are mean ± SD in MPa, N=16. Groups identified horizontally by different superscript letters are significantly different (p<0.05) (from Ito et al.52, with permission). +lc = with light-curing of each layer.