Skip to main content
. 2014 Oct 30;6(1):e959874. doi: 10.4161/21592527.2014.959874

Table 2.

Average grain size and mechanical properties of the as-received and annealed pure iron samples.

Material Average grain size (μm) Yield Strength (MPa) Tensile Strength (MPa) Elongation at break (%)
As-received 29.6 ± 4.0 170 ± 2 270 ± 5 49.3 ± 3.5
85%UR-550 14.1 ± 1.3 236 ± 13 287 ± 7 46.1 ± 4.2
75%UR-800 28.1 ± 2.9 104 ± 2 238 ± 5 47.0 ± 4.1
85%UR-1000 168.0 ± 28 93 ± 9 173 ± 17 17.2 ± 6.4