Mechanical properties of GH, GH-GlcN9 and GH-GlcN16 cryogels. Values are mean ± SD of five independent measurements.

GH GH-GlcN9 GH-GlcN16
Compressive elastic modulus, ε = 0.1 (kPa) 45.1 ± 5.3 30.3 ± 4.1 * 24.9 ± 3.6 *
Compressive elastic modulus, ε = 0.3 (kPa) 255.6 ± 77.9 156 ± 25.3 132.3 ± 19.8 *
Compressive strain to failure (%) 45.7 ± 1.5 49 ± 1.0 47.7 ± 3.1
Compressive stress to failure (kPa) 118.6 ± 12.1 90.6 ± 8.9 * 53.3 ± 5.0 *,#
Toughness (kJ/m3) 12.7 ± 1.3 10.8 ± 0.8 8.2 ± 2.1 *
Compression energy (kJ/m3) 2.5 ± 0.1 1.9 ± 0.3 * 1.3 ± 0.1 *,#
Relaxation energy (kJ/m3) 0.8 ± 0.1 0.7 ± 0.2 0.5 ± 0.1 *
Dissipation energy (kJ/m3) 1.7 ± 0.1 1.2 ± 0.1 * 0.8 ± 0.1 *,#
Percentage of energy dissipation (%) 68.2 ± 4.4 61.3 ± 1.4 * 59.7 ± 1.6 *

* p < 0.05 compared with GH cryogel; # p < 0.05 compared with GH-GlcN9 cryogel.