Table 2. Mean hardness values (VHN) (standard deviation) for the bottom surface of the resin cement specimens varying the curing light source and thickness of the indirect resin disks.
Resin diskt hickness (mm) | Light Source | Bottom* | % Difference Compared to 1 mm | % Difference** by curing light source and thickness |
1.0 | QTH | 19.1 (4.54)b | - | 67.5% |
1.0 | LED | 32.0 (3.28)ª | - | |
2.0 | QTH | 11.4 (4.67)b | -40.3% | 0.87% |
2.0 | LED | 11.5 (1.84)b | -64.1% | |
3.0 | QTH | 5.8 (1.60)b | -69.6% | 29.3% |
3.0 | LED | 7.5 (0.88)b | -76.6% |
The same superscripted letters indicate no significant differences (p > 0.05).
Absolute difference in mean VHN/ mean QTH VHN.