Table 3. Tensile testing of spidroin-like fibers.

Mean values for tensile properties and the corresponding standard deviations (STDEV) were recorded. Units for each parameter in the table are described in the column headers. Data for N. clavipes major ampullate (MA) silk comes from Gosline et al. [5].

Sample Sample Number Young's Modulus (MPa) Breaking Stress (MPa) Breaking Strain (unitless) Toughness
(J/cm^3)
mean STDEV mean STDEV mean STDEV mean STDEV
Sp1R8 Only 7 572 339 53 17 0.21 0.05 6.63 2.89
Sp1R8 & Amp 5 1465 671 53 11 0.08 0.02 2.56 1.15
Sp1R8 & Glut 9 4587 854 148 21 0.04 0.01 3.45 1.35
Sp2R8 Only 5 1220 853 67 21 0.20 0.07 8.07 0.55
Sp2R8 & Amp 5 1067 342 37 13 0.09 0.02 2.15 0.40
Sp2R8 & Glut 14 4500 1347 142 59 0.04 0.01 3.35 1.79
N. clavipes MA Silk 22000 1300 0.12 80