Overview of microwave treated solution A where the temperature and duration of the synthesis are represented in function of the particle size and crystallinity.

Temperature (°C) Duration (min) Particles size [a] (nm) Crystalline Present phase Crystallite size (nm)
140 5 37 No
140 60 47 Yes Monoclinic ZrO2 3.13 ± 0.11
150 5 45 Yes Monoclinic ZrO2 2.64 ± 0.11
150 30 52 Yes Monoclinic ZrO2 3.37 ± 0.10
160 5 50 Yes Monoclinic ZrO2 3.35 ± 0.10

[a] Secondary particle size is measured by DLS (dynamic light scattering).