Table 3.

Thermoelectric parameters of the most relevant conducting polymers at room temperature.

System σ(S·cm1) S (µV·K1) κ(W·m1·K1) PF (µW·m1·K2) ZT Refs.
PEDOT:Tos/ PEO-PPO-PEO electrochem. reduct. ∼1200 ∼100 1270 ∼1.02 [16]
PEDOT:PSS + EG treat. ∼980 ∼70 0.23 469 0.4 [48]
PEDOS-C6 electrochem. reduct. ∼200 ∼110 354.7 [83]
PEDOT:PSS + EG treat. + hydrazine reduct. ∼1300 ∼49 0.3 320 0.3 [13]
PEDOT:Tos + TDEA reduct. ∼80 ∼290 0.37 324 0.25 [13]
PEDOT:BTFMSI + hydrazine reduct. ∼1080 ∼37 0.19 147 0.22 [10]
PEDOT:PSS electrochem. reduct. ∼25 ∼90 0.17 23.5 0.041 [21]
PEDOT:PSS + DMSO 5% 298 12.65 4.78 ∼0.001 [44]
PANI/CSA-doping in m-cresol 220 ∼20 11 [25]
PANI doped with H3PO4 40 ∼7 0.19 [17]
polyselenophene and its copolymers with 3-methylthiophene 0.1–54 20–98 2–12 0.034 [38]
Copolymer of 1,12-bis(carbazolyl) dodecane and thieno[3,2-b]thiophene and its copolymers with 3-methylthiophene 4 × 105−0.4 75–169 ∼0.17–0.33 [52]
Phenylenevinylene block copolymers and their blends with MEH-PPV 6 × 106−14.4 7–531 ∼105–1.33 [45]
PEDOT:PSS + Polythiophenes Bilayered nanofilms 125–200 11–17 ∼1.5–6 [53]