SWCNT/PEDOT:PSS, DMSO, GA |
400 |
27 |
↑0.4 |
25 |
∼0.02 |
[56] |
CNT/PEDOT stabilizer TCPP |
980 |
70 |
|
500 |
|
[58] |
CNT/PVAc |
48 |
45 |
0.34 |
|
0.006 |
[55] |
SWCNT/PEDOT:PSS PVAc |
1000 |
41 |
0.2–0.4 |
160 |
|
[57] |
SWCNT/PEDOT:PSS Layered structure |
241 |
38.9 |
|
21.1 |
|
[84] |
SWCNT/PANI |
125 |
40 |
|
0.2 |
0.004 |
[59] |
3D-CNT/PANI |
40.35 |
23 |
0.29 |
|
0.0022 |
[59] |
CNT-PANI nanofibers |
15 |
10 |
|
0.16 |
0.0022 |
[85] |
PANI coated CNT/PANI |
28 |
21.6 |
0.4 |
|
0.001 |
[86] |
poly(3-hexylthiophene) SWCNTs |
1000 |
29 |
|
98 |
|
[61] |
MWCNT/polithiophene |
6 |
25 |
0.6 |
|
8.7 × 10−4
|
[87] |
PANI/graphite composites |
100 |
10 |
1.2 |
4.18 |
1.37 × 10−3
|
[63] |
PANI/graphene nanosheets pellet |
∼60 |
∼30 |
|
5.6 |
|
[64] |
PANI/graphene nanosheets film |
∼8 |
∼42 |
|
1.47 |
|
[64] |
PANI/graphene nanoplatelets mechanical blending |
123 |
34 |
|
14 |
|
[66] |
PEDOT:PSS/expanded graphite |
213 |
15 |
|
5.31 |
|
[68] |
PEDOT:PSS/graphene fullerene |
700 |
25 |
0.4 |
|
0.06 |
[69] |