System σ (S·cm1) S (µV·K1) κ (W·m1·K1) PF (µW·m1·K2) ZT Refs.
PEDOT:PSS PAA Bi2Te3 380 79 0.36 ∼240 0.2 [77]
PEDOT:PSS Bi2Te3 250 150 0.558 131 0.08 [74]
PANI Bi2Te3 nanorods p-type 11.626 39 0.11 1.8 0.004 [74]
PANI Bi2Te3 nanorods n-type 23 −70 10 [74]
PEDOT:PSS Bi2Te3 films 421 18.6 0.07 9.9 0.04 [76]
PEDOT:PSS Te 19.3 163 0.22–0.3 70.9 0.1 [78]
PEDOT:PSS Te nanowire ∼15 260 100 [79]
PEDOT:PSS Te nanowire ∼12 170 35 [80]
PEDOT:PSS Gold nanorod ∼2000 12 20 [80]
PH3T Bi2Te3 ∼4.5 118 6.3 [88]