Table 3.
Weight-to-Cement Ratio of Nanoinclusion 1 | Type of Cement-Matrix Composite 2 | Dispersion Technique | Increase Referred to OPC Specimen (%) 3 | References |
---|---|---|---|---|
0.3% GNPs; 40% FA; 5% SF | UHPC 4; Portland ASTM Type III | Bath Sonication; Polycarboxylate Superplasticiser | 45% Tensile Str.; 153% Energy Absorption | [146] |
0.3% CNFs; 40% FA; 5% SF | UHPC; Portland ASTM Type III | Bath Sonication; Polycarboxylate Superplasticiser | 56% Tensile Str.; 108% Energy Absorption | [146] |
1% CNTs | Mortar | CNT–COOH | 40% Compressive Str. | [137] |
0.15% CNTs; 30% SF | Mortar | CNT–COOH; CNT–OH 5 | 20% Compressive Str.; 50% Flexural Str. | [147] |
1.5% GO | Pavement Concrete | Polycarboxylate Superplasticiser | 48% Tensile Str. | [148] |
0.05% GO | Cement Paste | Polycarboxylate Superplasticiser | 40.4% Compressive Str.; 90.5% Flexural Str. | [149] |
0.05% GO | Mortar | Superplasticiser | 24.4% Compressive Str.; 70.5% Flexural Str. | [149] |
0.08% GO; 80% FA; 2% SF; 2% vol. PVA fibres | Mortar | Superplasticiser | 24.8% Compressive Str.; 37.7% Tensile Str.; 80.6% Flexural Str. | [150] |
1% GO | Mortar | Polycarboxylate Superplasticiser | 86.3% Compressive Str. | [151] |
1 GNPs: Graphite nanoplatelets, FA: Fly ash, SF: Silica fume, CNFs: Carbon nanofibres; 2 Unless otherwise specified, ordinary Portland cement ASTM Type I was used; 3 Specimens cured for 28 days; 4 Ultra high performance concrete; 5 Both functionalizations yielded similar results. Specimens cured for 14 days.