Alloy State σ02 (MPa) σUTS (MPa) e (%)
GC 89.8 101.0 0.4
GC + HT 87.8 126.0 2.0
SCL 79.7 134.8 0.9
SCL + HT 74.2 144.1 3.3
SCS 67.0 110.6 1.2
SCS + HT 67.6 133.5 4.4
ECAP 166.1 206.4 1.1
HT + ECAP 173.5 223.0 2.4