Skip to main content
. 2016 May 12;9(5):362. doi: 10.3390/ma9050362

Table 7.

Results of compressive strength tests.

Division Flowability (mm) Curing Compressive Strength (MPa) Average Compressive Strength (MPa)
Condition Period (day) 1 (min) 2 3 (max)
NSC Slump 163 ± 10 Steam curing 1 7 25.8 26.1 26.7 26.2
Air 2 7 13.3 13.8 14.1 13.7
28 24.8 25.3 25.9 25.3
UHPC Slump flow 680 ± 50 Steam curing 7 170.1 175.8 177.1 174.3
Air 7 103.4 105.7 109.8 106.3
28 126.5 127.5 128.3 127.4

1 High-temperature steam curing; 2 air dry curing.