Skip to main content
. 2015 Mar 27;8(4):1413–1427. doi: 10.3390/ma8041413

Table 4.

Characteristics of the studied pellets.

Property PO PS CP SW VS OB BS WS OP GP
M (% wb) 6.35 9.50 8.02 9.30 10.80 6.50 7.20 9.40 6.86 7.05
BD (kg/m3·wb) 678 675 697 650 700 582 644 * 620 780 824
DU (%) 95.41 97.20 96.79 98.20 98.80 97.50 95.50 94.40 91.41 85.83
C (% db) 50.94 51.80 50.50 50.50 46.90 47.02 43.85 45.10 51.42 42.97
H (% db) 6.34 5.70 5.80 6.10 5.70 7.62 5.50 6.00 6.56 9.28
N (% db) 1.81 0.37 0.43 0.48 0.58 0.34 0.77 0.91 1.98 2.05
S (% db) 0.10 0.03 0.03 0.03 0.05 0.00 0.10 0.00 0.10 0.17
Ash (% db) 2.48 2.50 4.81 0.90 7.10 3.32 10.51 9.10 5.55 7.47
HHV (MJ/kg·db) 19.30 19.70 21.41 20.80 18.70 18.82 17.43 18.25 22.03 19.54
LHV (MJ/kg·wb) 16.76 16.69 18.52 17.69 15.61 16.03 15.05 13.73 19.17 16.26
E (MJ/m3·wb) 13,363 11,267 12,907 11,496 10,927 9335 9695 8,510 14,954 13,396

* Bulk density in BS samples was obtained from Serrano et al. [15].