Skip to main content
. 2013 Jul 25;6(8):3139–3159. doi: 10.3390/ma6083139

Table 7.

Physical and mechanical characterization of concrete according to UNI EN 206-1.

Concrete Strength (MPa) Strength class UNI EN 206-1 Density [kg/m3] Density class UNI EN 206-1
CC 37.3 ± 1.6 30/33 (Not LC) 2245.8 ± 62 Not LC
CM1-45 22.5 ± 1.2 LC 20/22 1865.5 ± 41 D2.0
CM3-45 27.4 ± 1.1 LC 20/22 1897.3 ± 44 D2.0
CM4-45 22.6 ± 0.8 LC 20/22 1876.7 ± 50 D2.0
CM7-45 38.8 ± 1.0 LC 35/38 1927.9 ± 32 D2.0
CM9-45 41.8 ± 1.7 LC 35/38 1981.4 ± 71 D2.0
CM10-45 40.5 ± 1.5 LC 35/38 1938.6 ± 87 D2.0
CM1-35 18.9 ± 0.8 LC 16/18 1779.3 ± 22 D1.6
CM3-35 22.8 ± 0.9 LC 20/22 1797.2 ± 69 D1.6
CM4-35 17.4 ± 0.6 LC 12/13 1782.1 ± 51 D1.6
CM7-35 36.9 ± 1.2 LC 30/33 1912.8 ± 42 D2.0
CM9-35 39.6 ± 1.2 LC 35/38 1943.8 ± 88 D2.0
CM10-35 36.0 ± 0.9 LC 30/33 1924.8 ± 67 D2.0
CM1-55 7.2 ± 0.3 Nc 1750.1 ± 22 D1.6
CM3-55 11.4 ± 0.4 LC 8/9 1779.6 ± 43 D1.6
CM4-55 7.3 ± 0.4 Nc 1768.3 ± 52 D1.6
CM7-55 24.9 ± 0.5 LC 20/22 1854.5 ± 38 D2.0
CM9-55 28.8 ± 1.2 LC 25/28 1862.9 ± 62 D2.0
CM10-55 23.1 ± 0.9 LC 20/22 1879.2 ± 38 D2.0

CMx-y: means concrete made using AA prepared with the mixtures Mx and a plate revolution speed of y rpm; Nc: strength not classified.