Skip to main content
. 2017 Jul 20;7(7):187. doi: 10.3390/nano7070187

Table 3.

Fluidity, flexural strength, and compressive strength of ultra-high strength concrete (UHSC) with different content of GONSs. The UHSC samples containing 0.00%, 0.01%, and 0.03% bwoc GONSs are numbered as UGO00, UGO01, and UGO03, respectively.

No. Fluidity (mm) Flexural Strength (MPa) Compressive Strength (MPa)
Slump Slump Flow 7 d 7 d 28 d
UGO00 240 450 8.92 (0.00) 90.60 (0.00) 117.34 (0.00)
UGO01 235 420 9.98 (11.88) 93.92 (3.66) 126.52 (7.82)
UGO03 220 380 9.54 (6.95) 94.73 (4.55) 122.73 (4.59)