Table 1.
Summary of physical properties of the Fe3O4/PB nanocomposites.
| ρA g ∙ cm−³ | ρHe g ∙ cm−³ | P % | fm,poly weight-% | ENI GPa | HNI GPa | EB GPa | σB MPa | EC GPa | σC GPa | |
|---|---|---|---|---|---|---|---|---|---|---|
| Fe3O4@PB | 2.42 | 2.45 | 1.6 | 16.4 | 10.1 ± 0.4 | 0.21 ± 0.04 | 20 ± 5 | 191 ± 10 | 14 ± 1 | 369 ± 111 |
| Fe3O4@PB + S | 2.73 | 2.83 | 3.5 | 16.4 | 21.2 ± 1.5 | 0.83 ± 0.12 | 23 ± 8 | 184 ± 87 | 8 ± 2 | 476 ± 255 |
ρA: Archimedian density, ρHe: He-pycnometric density, fm,poly: mass fraction of polymer, E: elastic modulus measured by nanoindentation (NI), microbending (B) and microcompression (C) and σ: fracture strength of microbending (B) and microcompression (C).