Skip to main content
. 2017 Jul 1;10(7):736. doi: 10.3390/ma10070736

Table 1.

Preparation conditions, density, piezoelectric and dielectric parameters of the poled ceramics obtained by the solid state route.

Temp/Time Temp/Time Density d33 d31 Kp R.T. R.T.
Synthesis (°C/h) Sintering (°C/h) (g/cm3) (pC/N) (pC/N) (%) εT33 tan δ (%)
800/4 970/5 5.66 98 21 13 597 6
800/4 990/5 5.67 95 21 16 595 4
800/4 1000/5 5.79 20 5 4 591 40
800/1 1020/1 5.72 52 8 5 706 42
800/1 1050/1 5.65 68 18 13 642 5
800/1 1080/1 5.68 82 20 16 689 14