TABLE I.

Parameters for Production of Electrospun Polymer Nanofibers

Polymer FTY720 (w/w) Solvent Concentration (w/v) Working Distance (cm) Voltage (kV) Flow Rate (mL/hr)
PHB HFP 1.4 15 7 1.5
PHBV HFP 6.5 15–20 10 1
PCL THF:DMF 14 20 14 1
PLGA-PCL (1:1 w/w) 3:1 (v/v) chloroform: methanol 18 10 19 1
PLGA-PCL + FTY 1:200 3:1 (v/v) chloroform: methanol 20 15 19 1
PHBV-PCL (1:1 w/w) 3:1 (v/v) chloroform: methanol 18 14 19 1
PHBV-PCL + FTY 1:200 3:1 (v/v) chloroform: methanol 18 14 19 1