Preparation of PPF-HA printing solutions for bilayer and gradient scaffolds*

mPPF (g) VDEF (mL) HA BAPO
(g) (wt%) (mg) (wt%)
10 1.677 0 0 118.8 1
10 1.677 0.1489 1.25 240.1 2
10 1.677 0.3017 2.5 240.1 2
10 1.677 0.6192 5 240.1 2
10 1.677 1.3072 10 240.1 2
*

Considering PPF density (Mn 2530) ρPPF = 1.27 g/cm3 [35], and DEF density (Mn 172) ρDEF = 1.05 g/cm3 (Sigma Aldrich) at 25°C. mPPF= PPF mass, VDEF= DEF volume, wt% reported as xx+mPPF+VDEFρDEF100%