Mean diameters of PVDF nanofibers with different solution concentrations measured from SEM micrographs

Sample Solvent Concentration (w/v%) Voltage (kV) Distance (cm) Feeding rate (ml/h) Collector speed (rpm) Mean nanofiber diameter (nm)
S1 DMAC/acetone 10 15 14 0.7 1000 ***
S2 DMAC/acetone 20 15 14 0.7 1000 ***
S3 DMAC/acetone 25 15 14 0.7 1000 472.9 ± 21
S4 DMAC/acetone 30 15 14 0.7 1000 644.2 ± 29