Metals used in AM

Materials Printing technology Tensile strength, MPa Young's modulus, GPa Yield strength, MPa Relative density, % Thermal conductivity, W m−1 k−1 Max operating temperature, °C Ref.
Al/Si SLS, SLA 240–480 N/A 180–270 100 N/A 400 98, 99, 100
Co/Cr SLS 1200–1260 N/A 850–900 100 N/A 1150 101
NI/Cr SLS 1350 170 1075 100 11.4 650–980 102
Ti (alloy) SLS 450–1300 105–120 350–8000 100 6.7–26 425–540 26, 93, 103, 104, 105, 106
Stainless steel: 316L SLS 500–700 190 300–500 100 15–21 N/A 107
17–4 PH 1100–1300 N/A 620–1100 N/A N/A 550 108
Maraging steel 1100 N/A 860 N/A N/A 40 N/A 0 109
Alloy steel 300–600 N/A N/A 100 N/A 110
Cu Inkjet 3DP, SLS 116.7 N/A N/A 85.5 N/A N/A 111, 112