Table 1.
Thermal and mechanical properties of ABS-MOF-5 composites
| Glass Transition Temperature (°C) | Average values at breaking point
|
Young’s Modulus (MPa) | ||
|---|---|---|---|---|
| Stress (MPA) | Strain (%) | |||
| ABS | 106 | 39 ± 4 | 10 ± 1 | 5.2 ± 0.4 |
| 1% MOF-5 | 106 | 49 ± 4 | 12 ± 2 | 6.5 ± 0.7 |
| 5% MOF-5 | 105 | 39 ± 1 | 14 ± 2 | 4.0 ± 0.5 |
| 10% MOF-5 | 105 | 48 ± 1 | 11 ± 1 | 6.2 ± 0.4 |
| 20% MOF-5 | 105 | Composites at these percentages were unable to print structures for testing | ||
| 30% MOF-5 | 106 | |||
| 40% MOF-5 | 106 | |||
| 50% MOF-5 | 105 | |||