Mechanical properties of Sil-MA hydrogel depending on Sil-MA contents

Sil-MA contents (%) 10 20 30
Compressive stress at break (kPa) 122 ± 45 434 ± 128 910 ± 127
Compressive strain at break (%) 69.5 ± 0.5 77.7 ± 3.3 80 ± 5.1
Compressive elastic modulus at 50% strain (kPa) 17.7 ± 0.3 47.8 ± 4.8 125.8 ± 34
Tensile stress at break (kPa) ND 52 ± 4.3 75 ± 7.5
Elongation at break (%) ND 77.6 ± 3.8 124.2 ± 41
Tensile elastic modulus at 50% strain (kPa) ND 9.7 ± 1.0 14.5 ± 2.9
Water content at 5 h from dried Sil-MA (%) 4580 ± 480 2026 ± 202 1059 ± 121
Expansion rate at 5 h (%) 175.2 ± 6.1 150.0 ± 0.9 145.4 ± 2.4