Skip to main content
. 2018 Mar 27;11(4):504. doi: 10.3390/ma11040504

Table 4.

Mechanical properties of restorative composites after 7 days since curing, according to light source and curing mode. All the results are reported in terms of mean values and standard deviation (in brackets).

EPH DEI CLM SDR
LCU Elastic Modulus (MPa) Max. Stress (MPa) Max. Strain (%) Elastic Modulus (MPa) Max. Stress (MPa) Max. Strain (%) Elastic Modulus (MPa) Max. Stress (MPa) Max. Strain (%) Elastic Modulus (MPa) Max. Stress (MPa) Max. Strain (%)
Laser (Mode I) 8.6 (±0.7) 120.3 (±6.3) 2.2 (±0.1) 3.6 (±0.2) 61.9 (±4.1) 2.8 (±0.2) 6.0 (±0.7) 76.0 (±5.4) 1.4 (±0.1) 5.7 (±0.5) 107.5 (±5.9) 4.1 (±0.2)
Laser (Mode II) 8.4 (±0.8) 119.8 (±5.9) 2.1 (±0.2) 3.5 (±0.3) 60.2 (±4.8) 2.7 (±0.2) 5.9 (±0.5) 74.6 (±4.6) 1.4 (±0.1) 5.4 (±0.7) 105.8 (±6.1) 4.3 (±0.3)
LED Mectron (Mode I) 8.7 (±0.7) 121.9 (±5.8) 2.3 (±0.1) 3.8 (±0.2) 63.4 (±3.8) 2.9 (±0.1) 6.4 (±0.4) 77.8 (±4.3) 1.4 (±0.1) 5.7 (±0.4) 109.2 (±4.9) 4.4 (±0.2)
LED Enfis (Mode II) 8.1 (±0.7) 118.3 (±5.4) 2.2 (±0.1) 3.5 (±0.2) 56.7 (±5.3) 3.0 (±0.2) 6.3 (±0.5) 73.7 (±5.1) 1.3 (±0.1) 4.9 (±0.4) 93.0 (±6.8) 5.0 (±0.3)