Skip to main content
. Author manuscript; available in PMC: 2018 Jun 6.
Published in final edited form as: Stem Cells. 2011 Nov;29(11):1886–1897. doi: 10.1002/stem.746

Table 1.

Acrylamide and bisacrylamide concentrations used to make polyacrylamide gels with different Young’s moduli as measured by AFM. Values are means and 95% confidence intervals, n = 14.

Polyacrylamide gel formulations and corresponding Young’s Modulus

Acrylamide v/v % Bisacrylamide v/v % Young’s Modulus (Pa)
3 0.025 102 ± 2
3 0.04 207 ± 16
3 0.1 528 ± 11
4 0.05 692 ± 2
4 0.075 1498 ± 80
4 0.1 2123 ± 215
4 0.2 4018 ± 307
5 0.2 13365 ± 103
8 0.3 30567 ± 979
10 0.3 72904 ± 159
12 0.6 151002 ± 1498
15 1.2 292300 ± 528