Table 1.
Physicochemical properties of Cladophora nanocellulose and RSDAC beads. Adapted from Rocha et al. [18].
Physicochemical Properties | Cladophora Nanocellulose | RSDAC |
---|---|---|
Surface charged groups (μmol g−1) | 32 ± 2 a | 486 ± 5 b |
ζ-potential at pH 6.5 (mV) | −8 ± 3 | −25 ± 3 |
Specific surface area (m2 g−1) | 96 | 90 |
Total pore volume (cm3 g−1) | 0.44 | 0.20 |
Pore size distribution mode (nm) | 13 | 40 |
Beads size (µm) | - | 17 ± 5 |
a carboxyl groups, b sulfonate groups. Represents 48% of degree of sulfonation.