Skip to main content
. 2018 Jun 16;11(6):1028. doi: 10.3390/ma11061028

Table 3.

The tensile results of GFRP bars after cyclic load.

Temperature/°C Holding Time/h Cyclic Times Tensile Strength/MPa Elastic Modulus/GPa
25 / 0 810 55.1
4000 820 55.2
6000 802 54.5
100 0 0 815 54.3
4000 808 54.6
100 1 0 806 54.5
4000 802 53.9
100 2 0 800 54.4
4000 650 52.6
8000 585 54.7
150 0 0 806 53.2
4000 785 53.8
6000 762 53.4
200 0 0 777 52.5
4000 761 53.6
6000 748 53.6
200 1 0 763 54.1
4000 776 55.6
6000 755 53.1
8000 451 54.6
14,000 439 49.1
200 2 0 741 46.4
4000 666 45.7
6000 451 45.2
250 0 0 652 53.9
4000 576 53.6
300 0 0 646 51.8
4000 645 50.9
8000 460 50.7
300 1 0 638 49.7
4000 534 48.8
8000 495 48.0
10,000 469 46.8
350 0 0 630 48.3
4000 483 47.2
8000 401 45.4