entry | [SDS] (wt % rel to BA) | t (h) | conv (%) | b (h−1) | Mn,app (×10−3) | Mn,th (×10−3) | Đ | dZc (nm) |
---|---|---|---|---|---|---|---|---|
1 | 9.2 | 4 | 81 | 0.50 | 30.2 | 29.4 | 1.12 | 106 ± 2 |
2 | 4.6 | 6 | 66 | 0.25 | 30.9 | 24.4 | 1.17 | 117 ± 2 |
3 | 2.3 | 13 | 74 | 0.12 | 30.2 | 26.7 | 1.30 | 161 ± 1 |
4 | 1.15 | 20 | 74 | 0.16 | 35.2 | 27.2 | 1.32 | 207 ± 2 |
General conditions as in Table 1. [AsAc]/[CuII] = 0.5, AsAc injected dropwise at t = 0 h.
The linear slope of the ln([M]0/[M]) vs time in the first 10 h of polymerization.